USA EQUIVALENT PAPER WEIGHTS

In reams of 500 sheets, Basis weight in Bold type

Grade of Paper Book Bond Cover Bristol Index News-print TAG Grammage CALIPER
25 X 38 17 X 22 20 X 26 221/2X281/2 25 1/2 X 30 1/2 24 X 36 24 X 36 g/m2 Inch Point mm
Book 30 12 16 20 25 27 27 44  
40 16 22 27 33 36 36 59 0.0032 3.2 0.081
45 18 25 30 37 41 41 67 0.0036 3.6 0.092
50 20 27 34 41 45 45 74 0.0038 3.8 0.097
60 24 33 41 49 55 55 89 0.0048 4.8 0.120
70 28 38 47 57 64 64 104 0.0058 5.8 0.147
80 31 44 54 65 73 73 118 0.0061 6.1 0.155
90 35 49 61 74 82 82 133 0.0062 6.2 0.157
100 39 55 68 82 91 91 148 0.0072 7.2 0.183
120 47 66 81 98 109 109 178 0.0078 7.8 0.198
Bond 33 13 18 22 27 30 30 49  
41 16 22 27 33 37 37 61 0.0032 3.2 0.081
51 20 28 34 42 46 46 75 0.0038 3.8 0.097
61 24 33 41 50 55 56 90 0.0048 4.8 0.120
71 28 39 48 58 65 64 105 0.0058 5.8 0.147
81 32 45 55 67 74 74 120  
91 36 50 62 75 83 83 135 0.0068 6.8 0.173
102 40 56 69 83 92 93 151 0.0073 7.3 0.185
Cover 91 36 50 62 75 83 82 135 00.068 6.8 0.173
110 43 60 74 90 100 100 163 0.0074 7.4 0.188
119 47 65 80 97 108 108 176 0.0078 7.8 0.198
146 58 80 99 120 134 134 216 0.0092 9.2 0.234
164 65 90 111 135 149 149 243 0.0095 9.5 0.241
183 72 100 123 150 166 166 271 0.0110 11 0.289
201 79 110 136 165 183 183 298  
238 94 130 160 194 216 216 352  
292 115 160 197 239 266 266 433  
Vellum Bristol 99 39 54 67 81 90 90 147  
119 47 65 80 97 108 108 176  
148 58 81 100 121 135 135 219  
178 70 97 120 146 162 162 263  
207 82 114 140 170 189 189 307 0.011 11 0.275
237 93 130 160 194 216 216 351  
Index 110 43 60 74 90 100 100 163 0.0074 7.4 0.188
135 53 74 91 110 122 122 203 0.0085 8.5 0.216
170 67 93 115 140 156 156 252 0.0100 10 0250
208 82 114 140 170 189 186 328 0.0140 14 0.356
  269 106 147 181 220 244 244 398      
News-print 24 10 13 16 20 22 22 36      
  31 12 17 21 25 28 28 46      
  33 13 18 22 27 30 30 49      
  35 14 19 24 29 32 32 52      
  37 15 20 25 31 34 34 55      
  39 15 21 26 32 35 35 57      
TAG 110 43 60 74 90 100 100 163 0.0074 7.4 0.188
137 54 75 93 113 125 125 203 0.0090 9.0 0.229
165 65 90 111 135 150 150 244 0.0095 9.5 0.241
192 76 105 130 158 175 175 284 0.0130 13 0.330
220 87 120 148 180 200 200 326 0.0150 15 0.380
275 109 151 186 225 250 250 407  
  330 130 181 227 270 300 300 488      

To use the Weight Conversion tool, please select a Type of Paper from the pull down menu, then enter a value in pounds and hit calculate. To reverse the calculation simply select "gsmē->lbs" and enter a gsm value.

lbs -> g/mē g/mē->lbs

Type of Paper
lbs
Grams/Square meter
  Calculate

Point to Paper Weight Conversion (This is true for typical uncoated paper and assume 12 Pt. thick is equivalent to 270 gsm)

     

convert pt

to gsm
   
   
   
   

 

to mm
   
   
     

HOME| PULP| PAPER| CONVERTER| DISTRIBUTORS| CONSULTANT| MACHINERY| CONTROL | CHEMICAL | SCHOOL | ORGANIZATION| MAGAZINE| ENGINEERING CAL.| |EMPLOYMENT| DICTIONARY/GLOSSARY| ACRONYMS/ABBREVIATIONS | PAPER GRADES | PULP GRADES | RESOURCES | WASTE MANAGEMENT| PAPERMAKING| TESTING| REPAIR | LISTING| ADVERTISEMENT | SITE MAP|